Technical Specification for Evaluation of Salt Spray Test Chamber Results – Integrated Application Guideline based on GB/T 10125, GB/T 6461, ASTM B117 and ISO 9227

Source:LINPIN Time:2025-10-09 Category:Industry News

Scope and Purpose
Salt-spray corrosion testing is the core means of evaluating the resistance of materials and their protective coatings to chloride-containing environments. The test itself only provides an accelerated corrosion “stimulus”; the real technical value lies in the scientific evaluation of the test results. Improper choice of evaluation method or excessive operational error will directly lead to incorrect quality decisions, mis-estimation of service life and even market recalls. Taking current national/international standards as the backbone, this document systematically summarises four categories of result-evaluation methods for salt-spray test chambers and presents quantifiable error-control schemes for testing laboratories, in-house quality departments and third-party inspection bodies.
Salt Spray Test Chamber
Terms and Definitions
Substrate metal: the metallic body covered by a protective coating.
Protection rating (Rp): corrosion-resistance grade calculated from the percentage of corroded area; grade 0 is the worst, grade 10 the best.
Appearance rating (Ra): qualitative grade describing visible defects such as discoloration, loss of gloss or blistering.
Corrosion products: visible deposits formed by reaction between the substrate and the corrosive medium, e.g. white rust, red rust.
Systematic error: error component that remains constant or varies in a predictable way under the same conditions.
Result Evaluation Methods
3.1 Rating Method (Protection Rating Rp)
Field of application: quantitative assessment of pitting or general corrosion of the substrate after breakdown of protective coatings such as anodic films, electroplated layers or organic coatings.
Procedure:
a) At the end of the test gently rinse the specimens with de-ionised water to remove residual salt crystals.
b) Dry for 24 h at (23 ± 2) °C and (50 ± 5) % RH.
c) Examine with 7× magnification and 3 000 K white LED; record corroded area.
d) Convert to Rp using GB/T 6461, Table 1:
Rp = 10 – log10(A / 0.1), where A is the percentage of corroded area.
e) Take the arithmetic mean of three parallel specimens; if the range is ≥ 1 level, add two more specimens and re-test.
Acceptance criterion: typical automotive exterior parts require Rp ≥ 7; rail-transport structural parts require Rp ≥ 9. Customer specifications take precedence.
3.2 Gravimetric Method (Mass-Loss Method)
Field of application: metallic sheets or fasteners without protective coatings, or when uniform corrosion rate is required.
Procedure:
a) Before testing, degrease, acid-pickle, passivate and dry to constant mass (difference between consecutive weighings ≤ 0.1 mg).
b) Record initial mass m0 (accurate to 0.1 mg).
c) Test duration in accordance with the material standard, e.g. 48 h, 96 h, 240 h.
d) After testing, ultrasonically clean in 25 % HCl + 3 g/L hexamethylenetetramine for 10 min to remove corrosion products.
e) Dry to constant mass and record residual mass m1.
f) Calculate mass-loss rate Δm = (m0 – m1) / S·t, where S is exposed area (m2) and t is time (h); unit g/(m2·h).
Acceptance criterion: for 304 stainless steel Δm ≤ 0.1 g/(m2·h); for aluminium alloy 2A12 Δm ≤ 0.5 g/(m2·h) after 48 h.
3.3 Corrosion-Appearance Method (Go/No-Go Method)
Field of application: rapid screening, process comparison or on-site customer acceptance.
Procedure:
a) Photograph specimens immediately after test under ≥ 1 000 lx illumination.
b) Visual inspection is primary; use 5× magnification if necessary.
c) Record the first appearance time and morphology of white/red rust.
d) If the specification states “no substrate corrosion within 48 h”, any red rust means “fail”.
Precautions: because of subjectivity, at least two inspectors shall evaluate independently; if they disagree, a third arbitrator is introduced.
3.4 Statistical Analysis of Corrosion Data (Reliability Modelling Method)
Field of application: life prediction, estimation of corrosion-rate distribution and optimisation of sampling plans; not used for direct pass/fail judgement.
Procedure:
a) Collect ≥ 30 data points of corrosion depth or mass loss.
b) Use Anderson-Darling test to check for normal, log-normal or Weibull distribution.
c) Estimate distribution parameters by maximum likelihood and build cumulative distribution function F(t).
d) Calculate characteristic life T0.1 (time at 10 % failure probability) and its confidence interval.
e) Compare T0.1 with the required warranty life and evaluate design margin.
Output: a statement such as “At 95 % confidence the salt-spray resistance life is ≥ 720 h”, providing quantitative support for engineering improvement.
Error Sources and System Control
4.1 Chamber-Related Errors
Salt-fall-out rate deviation: standard requires (1.5 ± 0.5) mL/(80 cm2·h); outside this range corrosion kinetics shift exponentially.
Temperature gradient: a difference > 2 °C between any two points in the cabinet causes uneven condensate distribution.
pH drift: if collected solution pH is outside 6.5–7.2, chloride ion activity changes by > 15 %.
4.2 Correction and Reduction Measures
Metrological calibration: send the chamber every 12 months to a CNAS-accredited laboratory for calibration of temperature, fall-out rate and pH; obtain correction factor C and state expanded uncertainty U (k = 2) in the report.
Reference-sample substitution: insert two CR4 steel panels with known Rp = 9 in every test batch; if measured Rp deviates by > 1 level, multiply the whole batch by correction factor k = 9 / Rp(ref).
Symmetrical placement: if nozzle partial blockage is suspected, place specimens symmetrically about the cabinet centreline and average the left/right groups to cancel systematic offset.
Opposite-error compensation: run test A and test B on the same product; if A shows a positive “over-corrosion” error and B a negative “under-corrosion” error of similar magnitude, average the two Rp or Δm values as the best estimate.
Laboratory Management Requirements
Personnel: operators and evaluators must pass internal training and examination under GB/T 27025 and hold valid certificates; rating evaluations require two independent readings; if the difference is > 0.5 level a third arbitrator is introduced.
Equipment: chambers must have automatic water refill, low-level alarm and continuous fall-out recording; calibration labels must be valid.
Environment: evaluation area illumination 1 000–1 500 lx, colour-rendering index Ra ≥ 90; avoid direct sunlight.
Records: raw data shall be retained for ≥ 6 years and include test curves, photographs, correction factors and uncertainty budgets.
Worked Example
An aluminium alloy bracket (6063-T5) for a new-energy vehicle battery case was required to pass 720 h neutral salt spray. The supplier adopted a dual “rating + gravimetric” approach:
Rating result: Rp = 8.3 (customer limit ≥ 7).
Gravimetric result: Δm = 0.08 g/(m2·h) (customer limit ≤ 0.1).
Uncertainty: U = 0.4 level (k = 2), coverage factor k = 1.02.
Conclusion: pass; predicted warranty life T0.1 = 1 080 h, meeting the 5-year warranty requirement.
Closing Remarks
The evaluation results from a salt-spray test chamber are not only a “medical report” on material corrosion resistance but also the technical passport of a company’s quality reputation. Only by deeply integrating standard methods, statistical tools and error control can data be traceable, conclusions reproducible and risks predictable. Every laboratory should compile its own internal work instructions based on the framework above, adapt them to its equipment status and customer requirements, and periodically conduct proficiency testing to ensure continuous improvement of the technical credibility of salt-spray corrosion testing.

News Recommendation
Cold and hot shock test chambers utilize high-temperature and low-temperature zones during testing. In the testing process, two-box models involve placing the test product in high and low-temperature zones for cyclic exposure, while three-box models involve blowing high- and low-temperature gases onto the product alternately.
Cold and thermal shock test chamber on the market is divided into two categories, a two-compartment type, including high-temperature region and low-temperature region, the test object were tested in two different temperatures in the area of the test, alternating hot and cold test; the other is a three-compartment type, in addition to high-temperature and low-temperature areas, there is also a test area, and the difference between the two-compartment is that the three-compartment type does not need to be tested directly in the test area.
UV aging test chambers are crucial equipment for testing the weather - resistance performance of items under ultraviolet light conditions and are widely applied in numerous industries.
Different industries use rain test chambers for various testing purposes. What are these specific applications? Today, we’ll discuss them and also explore the installation requirements for such equipment.
In fact, waterproof testing in rain test chambers is divided into nine distinct levels. Below are the specifics of these nine levels
Product Recommendation
Telegram WhatsApp Facebook VK LinkedIn
亚洲欧美电影一区二区_麻豆国产一区二区_免费高清在线一区_久久免费高清视频
好吊一区二区三区| 欧美日韩美女一区二区| 亚洲一区二区视频在线观看| 亚洲伦理在线观看| 亚洲视频在线观看视频| 香蕉尹人综合在线观看| 久久天堂精品| 欧美日韩精品福利| 国产日韩欧美在线一区| 亚洲国产婷婷| 亚洲午夜精品| 免费观看国产成人| 国产精品九九| 国产一区二区三区高清在线观看 | 一区一区视频| 一本色道久久综合狠狠躁篇怎么玩| 亚洲资源av| 免费成人高清视频| 国产精品美女一区二区| 伊伊综合在线| 亚洲一区二区视频在线| 黄网站免费久久| 亚洲精品在线免费| 欧美一级一区| 欧美久久久久久久久| 国产亚洲视频在线观看| 亚洲乱码国产乱码精品精可以看| 亚洲欧美日韩国产综合| 免费看的黄色欧美网站| 国产精品黄色| 亚洲精品视频免费观看| 久久电影一区| 欧美性片在线观看| 亚洲激情欧美| 久久精品99| 国产精品国产三级国产专播精品人 | 国产精品亚洲成人| 亚洲精品欧美一区二区三区| 欧美自拍丝袜亚洲| 欧美特黄一级| 亚洲人成人一区二区三区| 久久精品99国产精品| 欧美性一二三区| 亚洲欧洲一区二区在线播放| 久久久国产成人精品| 国产精品久久久久久久久婷婷 | 久久嫩草精品久久久精品| 国产精品久久久久一区二区| 亚洲美女视频网| 久久手机精品视频| 国产亚洲欧美日韩美女| 亚洲一区二区三区在线观看视频| 欧美国产日本高清在线| 精品99视频| 久久激五月天综合精品| 国产精品社区| 亚洲图片在区色| 欧美裸体一区二区三区| 18成人免费观看视频| 久久精品国产在热久久| 国产精品一区一区三区| 亚洲一本视频| 欧美日韩国产区| 亚洲精品国产品国语在线app| 久久香蕉国产线看观看av| 国产一区二区三区四区| 欧美一区二区三区在线观看视频| 国产精品久久久久影院色老大| 99精品欧美一区| 欧美伦理影院| 亚洲免费av电影| 欧美精品一区二| 亚洲精品一区在线观看| 欧美激情第二页| 最新日韩在线视频| 欧美国产精品| 亚洲精品欧美激情| 欧美日韩美女在线| 在线视频欧美一区| 国产精品高精视频免费| 亚洲一区二区免费看| 国产精品swag| 亚洲永久网站| 国产午夜精品久久久| 久久国产毛片| 精品av久久707| 欧美a级一区二区| 日韩午夜免费| 欧美午夜精品久久久久久孕妇| 亚洲丝袜av一区| 国产精品入口| 欧美专区亚洲专区| 激情欧美一区二区三区在线观看 | 欧美日韩国产成人精品| 一本久道久久综合婷婷鲸鱼| 欧美日韩在线免费视频| 亚洲图片欧洲图片av| 国产精品美女xx| 欧美一区免费视频| 黄色综合网站| 欧美日本韩国一区二区三区| 一区二区日本视频| 国产精品麻豆欧美日韩ww | 国产精品久久亚洲7777| 欧美一级在线视频| 国内精品久久久久久久影视麻豆| 久久伊人亚洲| 亚洲伦理中文字幕| 国产精品豆花视频| 久久精品国产久精国产一老狼| 伊人久久亚洲美女图片| 欧美国产精品一区| 亚洲一区日韩在线| 韩国一区电影| 欧美顶级艳妇交换群宴| 亚洲手机成人高清视频| 国产一区二区欧美日韩| 玖玖国产精品视频| 99国产一区| 国产日韩欧美一区在线| 美女免费视频一区| 一区二区毛片| 国产中文一区二区| 欧美日本国产| 欧美在线免费视频| 亚洲精品欧美一区二区三区| 国产精品国产三级国产专播品爱网 | 亚洲视频在线免费观看| 国产一区二区三区日韩欧美| 农村妇女精品| 亚洲欧美日韩另类精品一区二区三区| 国语对白精品一区二区| 欧美连裤袜在线视频| 午夜精品一区二区三区在线播放| 影音先锋中文字幕一区二区| 欧美日精品一区视频| 久久国产日韩欧美| 日韩一区二区精品葵司在线| 国产亚洲欧美日韩日本| 欧美久久久久久蜜桃| 欧美在线观看一区二区| 日韩视频在线观看国产| 国产综合久久久久久| 欧美日韩成人一区| 久久久国产亚洲精品| 在线视频欧美日韩精品| 一区精品久久| 国产精品乱码久久久久久| 麻豆久久精品| 西瓜成人精品人成网站| 亚洲美女在线观看| 狠狠色丁香婷婷综合影院| 欧美香蕉大胸在线视频观看| 蜜桃av一区二区三区| 欧美亚洲日本网站| 一区二区精品国产| 亚洲高清中文字幕| 国产视频在线观看一区| 欧美日韩在线一区| 欧美jjzz| 久久久久久一区| 午夜精品久久久99热福利| 日韩亚洲一区二区| 在线观看欧美日韩| 国产午夜精品一区二区三区欧美| 欧美日韩在线精品一区二区三区| 美女成人午夜| 久久久精品动漫| 性娇小13――14欧美| 亚洲无线视频| 夜夜精品视频| 日韩视频在线观看| 亚洲国产精品久久久久婷婷老年 | 一区二区三区国产在线观看| 在线看成人片| 国产一区久久久| 国产欧美午夜| 国产精品区一区| 欧美午夜一区二区福利视频| 欧美激情一区二区三区在线视频| 久久深夜福利| 久久久www| 久久精品人人做人人爽电影蜜月| 午夜精品视频一区| 亚洲一二三四久久| 亚洲视频在线观看免费| 一区二区高清| 一本一本久久a久久精品综合妖精 一本一本久久a久久精品综合麻豆 | 久久爱另类一区二区小说| 亚洲伊人第一页| 亚洲视频一区在线| 一区二区三区.www| 夜夜嗨av一区二区三区网站四季av| 亚洲国产精品传媒在线观看 | 亚洲一区二区成人在线观看| 一本色道久久99精品综合| 一区二区av| 一区二区三区四区五区视频| 一本色道久久88综合日韩精品| aa国产精品| 在线综合亚洲| 亚洲综合久久久久| 午夜精品久久久久久99热软件| 午夜在线一区|